The critical dose for blister formation is 1. 5 multiplied by 10**1**9 ions/cm**2. A comparative study of Fe//4//0Ni//4//0P//1//4B//6 in amorphous and thermally crystallized states showed that the critical dose for blistering in the amorphous state is nearly three times higher than that in the crystallized state. TEM investigations revealed the precipitation of implanted hydrogen into gas bubbles in metallic glasses as well as the crystallized alloy.
引用
收藏
页码:72 / 75
页数:4