摘要
Loss of hardenability in the case was thought to be responsible for a lower than specified hardness found on a large carburized bushing. Pseudo Jominy testing on several high hardenability carburizing grades confirmed that hardenability fade was present at carbon levels above 0.65% and particularly for those steels containing molybdenum. Analysis of previous work provided a formula for calculating Jominy hardenability at various carbon levels. Again the results confirmed that the loss of hardenability was more severe in steels containing molybdenum.